Loctite EA 9390 AERO

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

Loctite EA 9390 AERO

Main features

  • Graphite- and Glass-Composite Repair
  • Hot/Wet Strength and High Shear Modulus
  • BMS 8-301 Heat-Cure Qualification

Product Description

LOCTITE® EA 9390 AERO Epoxy Paste Adhesive is a two-component, heat-curing epoxy developed for graphite- and glass-composite repair. The mixed adhesive has a typical viscosity of 100 Poise (10 Pa·s) at 77°F (25°C), supporting wetting and wet lay-up application. It combines good hot/wet strength with a high shear modulus and can be cured at temperatures from 200°F to 300°F (93°C to 149°C), depending on the required process schedule. The cured adhesive provides temperature-dependent lap shear performance on phosphoric-acid-anodized 2024-T3 bare aluminum and retains at least 1,000 psi (6.9 MPa) lap shear strength at an approximate service temperature above 350°F (177°C) under the stated ASTM D1002 test basis. The product is qualified to BMS 8-301.

Key features

  • Composite-repair formulation: Suitable as a wet lay-up resin for graphite- and glass-composite repairs.
  • Hot/wet mechanical performance: Combines good hot/wet strength with a high cured shear modulus.
  • Flexible heat-cure schedules: Supports documented cures at 200°F, 250°F, or 300°F (93°C, 121°C, or 149°C).

Applications / Suitable for

  • Graphite-composite repair
  • Glass-composite repair
  • Wet lay-up composite-repair processes
Product Family

LOCTITE EA 9390

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

Physical Properties
Viscosity (Part A)Viscosity (Part A)
94,000 mPa.s
Viscosity (Part B)Viscosity (Part B)
90 mPa.s
General Properties
Mix RatioMix Ratio
100:36

Additional Information

Technical properties

As-supplied / before-processing properties

Typical component, mixed-material, storage, and processing data for LOCTITE® EA 9390 AERO.

Property Value Unit Method / condition
Product type Two-component epoxy paste adhesive — As supplied
Part A color Light beige — Visual
Part B color Blue — Visual
Mixed color Violet — Visual
Part A viscosity 940 / 94 Poise / Pa·s 77°F / 25°C; Brookfield HBT, spindle 6 at 20 rpm / 2.1 rad/s
Part B viscosity 0.9 / 0.09 Poise / Pa·s 77°F / 25°C; Brookfield HBT, spindle 1 at 20 rpm / 2.1 rad/s
Mixed viscosity 100 / 10 Poise / Pa·s 77°F / 25°C; Brookfield HBT, spindle 3 at 10 rpm / 1.05 rad/s
Part A density 1.22 g/mL As supplied
Part B density 0.94 g/mL As supplied
Mixed density 1.15 g/mL Mixed material
Mix ratio, Part A:Part B 100:56 By weight Volume measurement is not recommended for structural applications unless ratio-control precautions are used
Pot life 2 hours 250 g mass at 77°F / 25°C; ASTM D2471, water bath
Recommended cured bondline thickness 3–6 / 0.08–0.15 mil / mm Documented application range
Cure schedule 220 at 200 / 93; 150 at 250 / 121; 130 at 300 / 149 minutes at °F / °C Alternative heat-cure schedules
Part A shelf life at ≤40°F / 4°C 1 year Stored at or below stated temperature
Part A shelf life at ≤77°F / 25°C 6 months Stored at or below stated temperature
Part A shelf life at ≤90°F / 32°C 2 months Stored at or below stated temperature
Part B shelf life 1 year At ≤40°F / 4°C, ≤77°F / 25°C, or ≤90°F / 32°C; refrigeration may cause crystallization
Technical properties

After-processing / final-state properties

Typical cured-material and bonded-joint properties. Values depend on the stated cure, specimen, conditioning, substrate, and test method.

Property Value Unit Method / condition
Tensile lap shear strength at −67°F / −55°C 2,200 / 15.2 psi / MPa ASTM D1002; cured 1 hour at 250°F / 121°C; 2024-T3 bare aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear strength at 77°F / 25°C 2,600 / 17.9 psi / MPa ASTM D1002; same specimen preparation and cure
Tensile lap shear strength at 180°F / 82°C 3,000 / 20.7 psi / MPa ASTM D1002; same specimen preparation and cure
Tensile lap shear strength at 250°F / 121°C 3,600 / 24.8 psi / MPa ASTM D1002; same specimen preparation and cure
Tensile lap shear strength at 300°F / 149°C 2,700 / 18.6 psi / MPa ASTM D1002; same specimen preparation and cure
Tensile lap shear strength at 350°F / 177°C 1,700 / 11.7 psi / MPa ASTM D1002; same specimen preparation and cure
Approximate service temperature >350 / >177 °F / °C Defined as temperature at which at least 1,000 psi / 6.9 MPa is retained by ASTM D1002
Tensile strength 8,200 / 56.5 psi / MPa ASTM D638; 0.125 in / 3.18 mm casting; tested at 77°F / 25°C
Tensile modulus 418 / 2,880 ksi / MPa ASTM D638; 0.125 in / 3.18 mm casting; tested at 77°F / 25°C
Elongation at break 2.5 % ASTM D638; tested at 77°F / 25°C
Shore D hardness 89 Shore D Tested at 77°F / 25°C
Glass transition temperature, dry 345 / 174 °F / °C Dry condition
Glass transition temperature, wet 302 / 150 °F / °C Wet condition
Shear modulus, dry 168 / 1,157 ksi / MPa Tested at 100°F / 38°C
Shear modulus after water conditioning 160 / 1,102 ksi / MPa Tested at 100°F / 38°C after 24 hours in water at 200°F / 93°C
Dielectric constant 4.19 — 1 kHz at 77°F / 25°C; ASTM D150
Dissipation factor 0.017 — 1 kHz at 77°F / 25°C; ASTM D150
Qualification BMS 8-301 qualified — Qualification stated for the exact product

Leading Brands Trust in Our Products and Services

  • Jabil
  • Linxens
  • Magna
  • Medtronic
  • NXP
  • Philips
  • Semikron
  • Teledyne
  • Thales
  • Vishay
  • ZF
  • AMS
  • Apple
  • Audi
  • Broadcom
  • Borgwarner
  • Bosch
  • Eaton
  • Henkel
  • Honeywell
  • Hysol
  • Intel
Products that Perform|Knowledge that Serves|Service that Delivers